Extrusion Processing Guide: PA 66 – Polyamide 66

1569
 Processing Guide: PA 66 – Polyamide 66
 Extruder: Single Screw Extruder
Without vacuum, plain feeding section
 Screw Design: Barrier Screw or Polyolefin Screw with equal feed ,transition and metering section, 25-30 L/D
 Compression Ratio: 3-4:1
 Cylinder Temperatures: 260-290°C
500-554°F
 Melt Temperature: 280-300°C
536-572°F
 Pre-Drying: 3 hours at 80°C (176°F) (very important)
 Calibration:  
 Miscellaneous: process above 250°C (482°F) to avoid freeze-off
if bubbles come then temperature too high
increased output/reduced wear by preheating of material 75°C (167°F) or by heating of feeding section at 160°C (320°F)
Note: This is meant as a general guide. Please consult your material and machinery representative.